Electroplating process for surface treatment of BGL towel rack products
(polishing→polishing)→hanging→degreasing and degreasing→water washing→(electrolytic polishing or chemical polishing)→pickling activation
→(pre-plating)→electroplating→washing→(post-treatment)→washing→drying→hanging→inspection and packaging
Ultrasonic: 4 minutes 3840L
Ultrasonic: 4 minutes 3840L
Washing: 2 minutes 1920L
Activation tank: 960L for 1 minute
Washing: 2 minutes 1920L
Ultrasonic: 4 minutes 3840L
Washing: 2 minutes 1920L
Activation tank: 1 minute 960L
Washing: 2 minutes 1920L
Copper chloride tank: 4800L in 5 minutes
1. Process
Washing: 2 minutes 1920L
Activation: 1 minute 960L
Washing: 2 minutes 1920L
General parameters of surface electroplating layer of zinc alloy pendant:
Chromium layer: 0.16μm
Copper layer: 11μm
Nickel layer: 4μm
PVD vacuum plating process
1. Hanging on the product
2. Put in ultrasonic degreasing and dewaxing for 10 minutes
3. Rinse with water for 5 times for 5 minutes
4. Dry the product
5. Put it in the oven to dry, and bake at low temperature for two hours
6. Then hang it into the vacuum ion furnace for 1 hour